Common defects
Ⅰ. Bubbles (Serious Defects)
Defect Identification: There are bubbles of varying sizes on the surface or inside the product, which form depressions when broken. They are commonly seen in the initial stage of extrusion or at the head of the profile, significantly affecting strength.
Causes: 1. There is a gap due to deviation in the fit between the extrusion cylinder, pad, and shaft; 2. Improper lubrication; 3. Excessive initial pressure during extrusion and unreasonable exhaust pressure; 4. High air content in the Aluminum Rod, cracks, or not meeting standards; 5. Inappropriate die clearance; 6. Oil stains and impurities on the extrusion cylinder.
Solutions: 1. Configure the extrusion pads according to specifications, and regularly inspect and replace worn parts; 2. Standardize lubrication and reduce the amount; 3. Slow down the initial pressure and set the exhaust pressure reasonably; 4. Inspect the Aluminum Rod according to YS/T67-1993 standards, and reduce speed and pressure when necessary; 5. Determine the die clearance based on tonnage; 6. Clean the extrusion cylinder at the end of each shift.

Ⅱ. Inclusions (Serious Defect)
Defect Identification: Foreign substances (such as ink, dust, etc.) are found on the surface or inside the product. This is commonly seen at the discharge head and can be observed with the naked eye, damaging the integrity of the product.
Causes: Surface contamination of the Aluminum Rod, impurities brought in during oil application, or unclean environment during compression, with debris entering the system.
Solutions: 1. Clean the surface of the Aluminum Rod before compression; 2. Protect the stored Aluminum Rods; 3. Standardize oil application to prevent contamination; 4. Maintain cleanliness of the workshop and equipment, and regularly clean the mold cavities.

Ⅲ. Color Difference (Extrusion Lines, General Defects)
Defect Identification: There are irregular color differences or strip-like lines on the product surface. These are more obvious after anodizing and do not affect strength but reduce the qualification rate of appearance.
Causes: 1. Uneven hardness and inconsistent wear on the working area of the mold; 2. The composition of the Aluminum Rod is uneven; 3. Unreasonable metal supply or mold cavity structure, resulting in turbulence.